Wafer #1552 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 10/4/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100.C-1LZ.0
- Lot Number: 1552
- Quantity Received: 320
- Manufacturer Test Report:
- Pore Size: 19%
- Porosity: 32.9 nm
- Flow Data Avg in SLPM
- 2psi: 0.163
- 4psi: 0..312
- Burst: 5.532
UR Testing
- Porosity: 12.89%
- Pore size: 60.9 +/- 14.92 nm
- Pore morphology: Standard
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Chip and Membrane Appearance – (Box-Folder: https://rochester.box.com/s/a4qz7vef9y29sxm9cren8c20w0j7pyln).
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- Representative membrane Image: See Below.

Experiences