Wafer #1514
Manufacturer’s Data
- Delivery Date: 11/21/2023 (picked up and logged by Ahmet Gurcan)
- Membrane Type: 1 Slot NPN
- SKU: NPSN100-1L
- Quantity Received: 290
- Manufacturer Test Report: Average porosity: 10.3%, Average pore size: 40.2nm
- Packing slip & invoice: None
UR Testing
- Porosity: N/A (Ran out before report was done)
- Pore size: N/A (Ran out before report was done)
- Pore morphology:
- Full Test Report / Images in Box:
- Chip and Membrane Appearance – some residue (Box Folder)
- Membrane dimensions (flat surface):
- EDS: Normal Si and N dominant
Experiences
- Cell culture
- Isabelle: Normal (HUVEC)
- Chloe: Normal (Human Astrocytes)
- Lananh: Normal (Primary rat: lung microvascular endothelial, Primary rat: alveolar epithelial cells.)
- Victor: iPSC-ECs fell off (too early to determine if its caused by membranes or cells themselves as of 12/5/2023)