Wafer #240803-11 – 2 Slot NPN
Manufacturer’s Data
- Delivery Date: 12/18/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 2 Slot
- SKU: NPSN100-2LWMS
- Lot Number: 240803-11
- Quantity Received: 270
- Manufacturer Test Report:
- Pore Size: 50.9 nm
- Porosity: 14.2%
- Flow Data Avg in SLPM
- 2psi: 0.334
- 4psi: 0.672
- Burst: 5.144
UR Testing
- Porosity: 14.06%
- Pore size: 51.54 +/- 13.98 nm
- Pore morphology: Standard
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Chip and Membrane Appearance – (Box-Folder: https://rochester.box.com/s/7ihwkajpbcx873vpjmj2nke2mvr6s3n1).
- Membrane dimensions (flat surface): 2 x (0.7 mm x 2 mm)
- Representative membrane Image: