Wafer #240917-01 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 4/29/2025 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100.C-1LZ.0
- Lot Number: 240917-01
- Quantity Received: 280
- Manufacturer Test Report:
- Pore Size: 64.4 nm
- Porosity: 18.2%
- Flow Data Avg in SLPM
- 2psi: 0.095
- 4psi: 0.19
- Burst: 8.211 PSI
UR Testing
- Porosity: 9.11%
- Pore size: 53.65 +/- 19.2 nm
- Pore morphology: Standard
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- For more information visit: https://rochester.box.com/s/2kz9xppuesnnfggd69il6n4e0ozx2y0a