Wafer #240803-12 – 1 Slot NPN

Manufacturer’s Data

  • Delivery Date: 12/18/2024 (picked up and logged by Ahmet Gurcan)
  • Membrane Type:  NPN 1 Slot
  • SKU: NPSN100.C-1LZ.0
  • Lot Number: 240803-12
  • Quantity Received: 320
  • Manufacturer Test Report:
    • Pore Size: 50.5 nm
    • Porosity: 11.6
    • Flow Data Avg in SLPM
      • 2psi: 0.16
      • 4psi: 0.307
      • Burst: 4.919

UR Testing

  • Porosity: 9.99%
  • Pore size: 50.62 +/- 14.61 nm
  • Pore morphology: Standard
  • EDS: N/A
  • 3 Membranes from this lot were removed for QC measurements.
  • Chip and Membrane Appearance – (Box-Folder: https://rochester.box.com/s/ro0mh943ni6e7yapsw8e6glq3uk52e3u).
  • Membrane dimensions (flat surface): 0.7 mm x 2 mm
  • Representative membrane Image: See Below.

 