Wafer #240803-13 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 12/18/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100.C-1LZ.0
- Lot Number: 240803-13
- Quantity Received: 250
- Manufacturer Test Report:
- Pore Size: 48.7 nm
- Porosity: 14.7%
- Flow Data Avg in SLPM
- 2psi: 0.168
- 4psi: 0.32
- Burst: 4.945
UR Testing
- Porosity: 13.45%
- Pore size: 50.66 +/- 14.14%
- Pore morphology: Standard
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Chip and Membrane Appearance – (Box-Folder: https://rochester.box.com/s/lsgii5qw6ngws12pwx7xu0inyg0adqhq).
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- Representative membrane Image: See Below.