Wafer #240803-09 – 2 Slot NPN

Manufacturer’s Data

  • Delivery Date: 12/18/2024 (picked up and logged by Ahmet Gurcan)
  • Membrane Type:  NPN 2 Slot
  • SKU: NPSN100-2LWMS
  • Lot Number: 240803-09
  • Quantity Received: 20
  • Manufacturer Test Report:
    • Pore Size: 51.8 nm
    • Porosity: 13.5%
    • Flow Data Avg in SLPM
      • 2psi: 0.304
      • 4psi: 0.584
      • Burst: 4.882

UR Testing

  • Porosity: 11.72%
  • Pore size: 52.42 +/- 15.33 nm
  • Pore morphology: Standard
  • EDS: N/A
  • 3 Membranes from this lot were removed for QC measurements.
  • Chip and Membrane Appearance – (Box-Folder: https://rochester.box.com/s/fta416emzuaoe4gezs08bq4qpc3vxoz9 ).
  • Membrane dimensions (flat surface): 2 x (0.7 mm x 2 mm)
  • Representative membrane Image:

 