Wafer #240919-25 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 4/28/2025 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100.C-1LZ.0
- Lot Number: 240919-25
- Quantity Received: 370
- Manufacturer Test Report:
- Pore Size: 67.3 nm
- Porosity: 22.8%
- Flow Data Avg in SLPM
- 2psi: 0.072
- 4psi: 0.137
- Burst: 5.789 PSI
UR Testing
- Porosity: 11.11%
- Pore size: 61.58 +/- 15.52 nm
- Pore morphology: Standard
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Membrane dimensions (flat surface): 0.7 mm x 2 mm