Wafer #1523 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 2/28/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100-1L-TE
- Lot Number: 1523
- Quantity Received: 237
- Manufacturer Test Report:
- Pore Size: 52.7nm
Porosity: 15.0%
Flow Data Avg in SLPM
2psi: 0.126
4psi: 0.276
Burst: 6.151
- Pore Size: 52.7nm
- Packing slip & invoice: None
UR Testing
- Porosity: 13.7 +/- 0.5%
- Pore size: 54.2 +/- 1.5 nm
- Pore morphology: Slightly under etched
- EDS: N/A
- Chip and Membrane Appearance – (Box Folder: https://rochester.box.com/s/cm987ibxh8nlzdtkheiu0w3svsy0nw0v)
- TEM Images: https://rochester.box.com/s/mio7alw4bkl6o4b68nrx6vy00wj4xte6
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- Representative membrane image: See Below.


Experiences
- Cell culture
- Lananh is having issues with cell culture as of 3/25/2024 with this lot
- The issue was not with the lot, but rather the cells (4/15/2023).
- Lananh is having issues with cell culture as of 3/25/2024 with this lot