Wafer #1531 – 3 micron Dual Scale – High Porosity
Manufacturer’s Data
- Delivery Date: 3/14/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 3 micron Dual Scale High Porosity
- SKU: DSSN100-1L-10%-3.0
- Lot Number: 1531
- Quantity Received: 315
- Manufacturer Test Report:
Avg Porosity: 15.1%Avg Nano Pore diameter:50.7nmAvg Micro Pore diameter: 2.986umAvg flux SLPM at 1PSI: 0.445Avg flux SLPM at 2PSI: 0.720Avg Burst Pressure: 3.493
- Packing slip & invoice: None
UR Testing
- Nano porosity: 12.2 +/- 0.6%
- Microporosity: 10.88%
- Nanopore size: 49.9 +/- 1.0 nm
- Micropore size: 2.905 μm
- Pore morphology: Standard
- EDS: N/A
- Chip and Membrane Appearance:
- Box Folder with more images :https://rochester.box.com/s/ou1te1jdii9hfutysobsl0k8sehlscyo)
- TEM Images: https://rochester.box.com/s/ufhc59h6jbkya71ctyef5ae2kvb0oxtk
- SEM Images of membranes: https://rochester.box.com/s/aygjy5qph8wey4ltw5ccmlo0pr2n12f5
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- Representative Membrane Image: See Below


Experiences
- Cell culture
- N/A as of 3/14/2024