Wafer #1532 – 2 Slot Wide NPN
Manufacturer’s Data
- Delivery Date: 3/14/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: 2 Slot NPN – Wide
- SKU: NPSN100-2LWMS
- Lot Number: 1532
- Quantity Received: 299
- Manufacturer Test Report:
- Avg Porosity: 13.4%
- Avg Pore diameter: 48.7nm
- Avg flux SLPM at 2PSI: 0.244
- Avg flux SLPM at 4PSI: 0.462
- Avg Burst Pressure: 6.564
- Packing slip & invoice: None
UR Testing
- Porosity: 10.9 +/- 1.8 %
- Pore size: 54.0 +/- 4.3 nm
- Pore morphology: Standard
- EDS: N/A
- Chip and Membrane Appearance:
- Some specs on membrane area occasionally.
- Box Folder with more images : https://rochester.box.com/s/xjjpnujrewyacs6r6i3xvhpbwxzdieul)
- Membrane dimensions (flat surface): 2 x 0.7 mm x 2 mm
- Representative Membrane Image: See Below


Experiences
- Cell culture
- N/A as of 3/14/2024