Manufacturer’s Data
- Delivery Date: 4/5/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: 0.5-micron microslit
- SKU: MSSN400-3L-0.5
- Lot Number: 5150
- Quantity Received: 180
- Manufacturer Test Report:
- Calculated Specs:
- Porosity: ~10.1%
- Slits/Membrane: 6820
- Slit Length: 50um
- Measured Specs:
- Avg. Slit Width: 0.47um
- Avg. Flow @ 2 PSI: 1.142 SLM
- Avg. Burst Pressure: 8.2 PSI
- Calculated Specs:
- Packing slip & invoice: None
UR Testing
- Porosity: N/A
- Pore size: N/A
- Pore morphology: N/A
- EDS: N/A
- Chip and Membrane Appearance
- Box Folder with more images : https://rochester.box.com/s/6c8rneszhurdptvbq4e6s3rcew8ceht1)
- Membranes have some stain like debris outside of the window area.
- Membrane dimensions (flat surface): 3 x 0.7 mm x 2.5 mm
- Representative Membrane Image: See Below