Wafer #240919-13 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 3/26/2025 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 2 Slot Wide Short
- SKU: NPSN100.C-2LZ.4
- Lot Number: 240919-13
- Quantity Received: 150
- Manufacturer Test Report:
- Pore Size: 63.2 nm
- Porosity: 22.9%
- Flow Data Avg in SLPM
- 2psi: 0.314
- 4psi: 0.594
- Burst: 6.899 PSI
UR Testing
- Porosity: 12.09%
- Pore size: 55.25 +/- 13.24 nm
- Pore morphology: Standard
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- For more information visit: https://rochester.box.com/s/5o3e80ywvvhyjkl88cs5ntp636jat8me
Experiences