Wafer #2400603-13 – 3 μm Dual Scale – Low Porosity (High Porosity)
Manufacturer’s Data
- Delivery Date: 12/8/2023 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 3 micron Dual Scale
- SKU: DSSN100-1L-3.0-A1 (0.625% Porosity – Not real porosity)
- Lot Number: 2400603-13
- Quantity Received: 320
- Manufacturer Test Report:
- Average (NPSN) Porosity: 7.7%
- Average (DSSN) Porosity: NA
- Average Diameter: 66.8 +/- 1.67 nm
- Packing slip & invoice: None
UR Testing
- Average Porosity (NPSN): NA
- Average Porosity (DSSN): 9.1%
- Pore size: 2.63 micron
- Pore morphology: Standard
- EDS: N/A
- Chip and Membrane Appearance:
- Window is highly clean. Outside of the window might have some shards from the cutting process and has some white scratches and digs.
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- Full Test Report / Images in Box: See Below for Image:
- Representative Box Image: See Below
Experiences: THIS PRODUCT WAS FOUND TO BE HIGH POROSITY ~9%