Wafer #240919-05 – 3 μm Dual Scale – Low Porosity
Manufacturer’s Data
- Delivery Date: 2/5/2025 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 3 micron Dual Scale
- SKU: DSSN100-1L-3.0-A1 (0.625% Porosity – Not real porosity)
- Lot Number: 240919-05
- Quantity Received: 230
- Manufacturer Test Report:
- Average Porosity (nanoporosity): 31%
- Average Diameter (microporous): 2.84 μm
- Average Diameter (nanoporous): 48.8 nm
- Average Flux @ 1 PSI: 0.167
- Average Flex @ 2 PSI: 0.299
- Average Burst Pressure (PSI): 2.45
- Packing slip & invoice: None
UR Testing
- Average Porosity (nanoporosity): 17.28%
- Average Porosity (microporoisty):
- Pore Size (nanopores): 70.18 +/- 19.07 nm
- Pore Size (micropores):
- Pore morphology: Standard
- EDS: N/A
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- For more information visit: https://rochester.box.com/s/mqhf1jdz5li17cbh9250og45onh59twp
Experiences: