Wafer #1548 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 7/26/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100.C-1LZ.0
- Lot Number: 1548
- Quantity Received: 300
- Manufacturer Test Report:
- Pore Size: 47.9 nm
- Porosity: 12.6%
- Flow Data Avg in SLPM
- 2psi: 0.081
- 4psi: .164
- Burst: 5.111
UR Testing
- Porosity: 7.5+/- 0.65%
- Pore size: 45.5 +/- 1.6 nm
- Pore morphology: 0.86 +/- 0.01 circularity
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Chip and Membrane Appearance – (Box-Folder: https://rochester.box.com/s/0sy64hluuxepk0qroh325au06y12ue1l).
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- Representative membrane Image: See Below.

Experiences