Wafer #1549 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 7/26/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100.C-1LZ.0
- Lot Number: 1549
- Quantity Received: 300
- Manufacturer Test Report:
- Pore Size: 57.8 nm
- Porosity: 14.1%
- Flow Data Avg in SLPM
- 2psi: 0.102
- 4psi: 0.194
- Burst: 5.617
UR Testing
- Porosity: 7.3+/- 0.5%
- Pore size: 53.55 +/- 2.65 nm
- Pore morphology: 0.82 +/- 0.02 circularity
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Chip and Membrane Appearance – (Box-Folder: https://rochester.box.com/s/18tgf5oi5ixqgt7t28pltla3y8qfop4j).
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- Representative membrane Image: See Below.