Wafer #1534 – 2 Slot Wide NPN
Manufacturer’s Data
- Delivery Date: 9/11/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: 2 Slot NPN – Wide
- SKU: NPSN100-2LWMS
- Lot Number: 1534
- Quantity Received: 30
- Manufacturer Test Report:
- Avg flux SLPM at 2PSI: 0.22
- Avg flux SLPM at 4PSI: 0.44
- Avg Burst Pressure: 4.75
- Average porosity: 10.1%
- Avg pore size: 42 nm
- Packing slip & invoice: None
UR Testing
- Porosity: 11.93%
- Pore size: 47.58 +/- 12.64 nm
- EDS: N/A
- Chip and Membrane Appearance
- Box Folder with more images https://rochester.box.com/s/s2iexa1sskl7lzwe1z43sdi5cgroktia
- Membrane dimensions (flat surface): 2 x 0.7 mm x 2 mm
- Representative Membrane Image:
Experiences
- Cell culture
- N/A as of 9/11/2024