Wafer #1538 – 2 Slot Wide NPN
Manufacturer’s Data
- Delivery Date: 9/11/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: 2 Slot NPN – Wide
- SKU: NPSN100-2LWMS
- Lot Number: 1538
- Quantity Received: 200
- Manufacturer Test Report:
- Avg flux SLPM at 2PSI: 0.438
- Avg flux SLPM at 4PSI: 0.462
- Avg Burst Pressure: 5.184
- Average porosity: 14%
- Avg pore size: 45.4 nm
- Packing slip & invoice: None
UR Testing
- Porosity: 8.5%
- Pore size: 39.74 +/- 11.89 nm
- EDS: N/A
- Chip and Membrane Appearance
- Box Folder with more images https://rochester.box.com/s/fzzdh54247eamcp2xe0elcmijwrqigv9
- Membrane dimensions (flat surface): 2 x 0.7 mm x 2 mm
- Representative Membrane Image:
Experiences
- Cell culture
- N/A as of 9/11/2024