Wafer #240919-14 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 6/4/2025 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100.C-1LZ.0
- Lot Number: 240919-14
- Quantity Received: N/A
- Manufacturer Test Report:
- Pore Size: 63.8 nm
- Porosity: 24.5%
- Flow Data Avg in SLPM
- 2psi: 0.15
- 4psi: 0.287
- Burst: 7.185 PSI
UR Testing
- Porosity: 12.45%
- Pore size: 57.92 +/- 16.09 nm
- Pore morphology: Standard
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Membrane dimensions (flat surface): 0.7 mm x 2 mm