Wafer #1537 – 2 Slot Wide NPN
Manufacturer’s Data
- Delivery Date: 3/26/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: 2 Slot NPN – Wide
- SKU: NPSN100-2LWMS
- Lot Number: 1537
- Quantity Received: 300
- Manufacturer Test Report:
- Avg flux SLPM at 2PSI: 0.197
- Avg flux SLPM at 4PSI: 0.374
- Avg Burst Pressure: 4.589
- Average porosity: 11.8%
- Avg pore size: 48.1nm
- Packing slip & invoice: None
UR Testing
- Porosity: 8.8 +/- 0.8%
- Pore size: 49.1 +/- 2.4 nm
- Pore morphology: Underetched
- EDS: N/A
- Chip and Membrane Appearance
- Box Folder with more images :https://rochester.box.com/s/mrfzd2lbjxow7v4l8tmhlggdip50n7vthttps://rochester.box.com/s/992hfckiw8xj4ggx8iiffa6li7t7twc8)
- Some scratches on the surface, some silicone debris from cutting process are also on outer edges of the frame. These should not cause issues and these are merely cosmetic defects
- Membrane dimensions (flat surface): 2 x 0.7 mm x 2 mm
- Representative Membrane Image: See Below


Experiences
- Cell culture
- N/A as of 3/26/2024