Wafer #24240803-19 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 6/3/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100.C-1LZ.0
- Lot Number: 24240803-19
- Quantity Received: N/A
- Manufacturer Test Report:
- Pore Size: 46.5 nm
- Porosity: 11.3%
- Flow Data Avg in SLPM
- 2psi: 0.132
- 4psi: 0.262
- Burst: 5.497 PSI
UR Testing
- Porosity: 11.52%
- Pore size: 54.25 +/- 15.63 nm
- Pore morphology: Standard
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- For more information visit: https://rochester.box.com/s/tslg4txawzt79f3pl8g896cwtsu6tztk