Wafer #1515 – 1 Slot NPN

Manufacturer’s Data

  • Delivery Date: 1/11/2024 (picked up and logged by Ahmet Gurcan)
  • Membrane Type:  NPN 1 Slot
  • SKU: NPSN100-1L
  • Lot Number: 1515
  • Quantity Received: 305
  • Manufacturer Test Report:
    • Avg Porosity: 13.5%
    • Avg Pore diameter: 39.2mn
    • Avg flux SLPM at 2PSI:  0.105 PSI
    • Avg flux SLPM at 4PSI:  0.215 PSI
    • Avg Burst Pressure:  5.141 PSI
  • Packing slip & invoice: None

UR Testing

  • Porosity: 13.2 ± 0.5
  • Pore size:  46.5 ± 1.3
  • Pore morphology: Standard
  • EDS: N/A
  • Chip and Membrane Appearance – (Box Folder: https://rochester.box.com/s/xqx2ub36q7tm5eqdtuwj98cilmsajth7). Some small debris on surface of membranes.
  • Membrane dimensions (flat surface): 0.7 mm x 2 mm
  • Full Test Report / Images in Box: See Below
  • Representative Box Image: See Below.

 

Experiences

  • Lananh is having issues with cell culture as of 3/25/2024 with this lot
  • No other issues reported