Are all fields created equal?

I’ve always wondered what the variability was in the pore statistics extracted from TEM images of different fields on the same membrane (SC 141).  I took a series of ten images from random positions (corners, edges, center) and ran them through the pore processor.  Here are the results:

(images taken at 100 kx)

position porosity cutoff [nm]
1 6.74% 19.6
2 6.58% 19.4
3 6.97% 19.6
4 6.64% 19.4
5 6.95% 19.6
6 7.08% 19.7
7 7.00% 19.4
8 6.92% 19.6
9 6.78% 19.5
10 6.79% 19.7
avg 6.85% 19.55
std dev 0.16% 0.12

I think it’s safe to say that statistics from one location on the membrane is representative of the entire film.