Wafer #240803-16 – 3 μm Dual Scale – Low Porosity
Manufacturer’s Data
- Delivery Date: 12/20/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 3 micron Dual Scale
- SKU: DSSN100-1L-3.0-A1 (0.625% Porosity – Not real porosity)
- Lot Number: 2408603-16
- Quantity Received: 320
- Manufacturer Test Report:
- Average Porosity (nanoporosity): 13.5%
- Average Diameter (microporous): 2.837 μm
- Average Diameter (nanoporous): 48 nm
- Average Flux @ 1 PSI: 0.163
- Average Flex @ 2 PSI: 0.285
- Average Burst Pressure (PSI): 3.77
- Packing slip & invoice: None
UR Testing
- Average Porosity (NPSN): 15.76%
- Average Porosity (DSSN):
- Pore size: 62.81 +/- 17.89 nm
- Pore morphology: Standard
- EDS: N/A
- Chip and Membrane Appearance:
- Window is highly clean. Outside of the window might have some shards from the cutting process and has some white scratches and digs.
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- For more information visit: https://rochester.box.com/s/dkd36t2ewi3sfwyqnptt6406vps449n3