Wafer #1525 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 5/20/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100-1L
- Lot Number: 1524
- Quantity Received: 310
- Manufacturer Test Report:
- Pore Size: 53.3 nm
- Porosity: 15.3%
- Flow Data Avg in SLPM
- 2psi: 0.112
- 4psi: .252
- Burst: 5.393
- Packing slip & invoice: https://rochester.box.com/shared/static/cu12kq9z92q42qio1jueh89m0jhbvke7.pdf
UR Testing
- Porosity: 12.5 +/- 0.95%
- Pore size: 59.5 +/- 1.5 nm
- Pore morphology: 0.86 +/- 0.02 circularity
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurments
- Chip and Membrane Appearance – (Box-Folder: https://rochester.box.com/s/inrx2wktj6hejlm5h7eifrvzwy7lilhc).
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- Representative membrane Image: See Below.

Experiences
- Cell culture (none as of 6/20/2024)