Wafer #240803-03 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 12/3/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100.C-1LZ.0
- Lot Number: 240803-03
- Quantity Received: 350
- Manufacturer Test Report:
- Pore Size: 16.9%
- Porosity: 56.4 nm
- Flow Data Avg in SLPM
- 2psi: .169
- 4psi: 0.343
- Burst: 3.551
UR Testing
- Porosity: 13.83%
- Pore size: 55.6 +/- 14.8
- Pore morphology: Standard
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Chip and Membrane Appearance – (Box-Folder: https://rochester.box.com/s/j5h2bt3h7dlg01sxd4ajb61dgg38o2bc).
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- Representative membrane Image: See Below.