Wafer #240919-01 – 3 μm Dual Scale – Low Porosity

Manufacturer’s Data

  • Delivery Date: 2/5/2025 (picked up and logged by Ahmet Gurcan)
  • Membrane Type:  NPN 3 micron Dual Scale
  • SKU: DSSN100-1L-3.0-A1 (0.625% Porosity – Not real porosity)
  • Lot Number: 240919-01
  • Quantity Received: 180
  • Manufacturer Test Report:
    • Average Porosity (nanoporosity): 28%
    • Average Diameter (microporous): 2.88 μm
    • Average Diameter (nanoporous): 49.4 nm
    • Average Flux @ 1 PSI: 0.134
    • Average Flex @ 2 PSI: 0.233
    • Average Burst Pressure (PSI): 2.504
  • Packing slip & invoice: None

UR Testing

  • Average Porosity (nanoporosity): 8.57%
  • Average Porosity (microporoisty):
  • Pore Size (nanopores): 53.41 +/- 15.31 nm
  • Pore Size (micropores):
  • Pore morphology: Standard
  • EDS: N/A
  • Chip and Membrane Appearance:
  • Membrane dimensions (flat surface): 0.7 mm x 2 mm
  • For more information visit: https://rochester.box.com/s/jx87khyye9minu5q4yct2ofo5lm6iwj8

 

Experiences:

Similar Posts