Wafer #240919-02 – 3 μm Dual Scale – Low Porosity
Manufacturer’s Data
- Delivery Date: 2/5/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 3 micron Dual Scale
- SKU: DSSN100-1L-3.0-A1 (0.625% Porosity – Not real porosity)
- Lot Number: 240919-02
- Quantity Received: 200
- Manufacturer Test Report:
- Average Porosity (nanoporosity): 27.2%
- Average Diameter (microporous): 2.84 μm
- Average Diameter (nanoporous): 49.2 nm
- Average Flux @ 1 PSI: 0.151
- Average Flex @ 2 PSI: 0.255
- Average Burst Pressure (PSI): 2.207
- Packing slip & invoice: None
UR Testing
- Average Porosity (nanoporosity): 17.17%
- Average Porosity (microporoisty):
- Pore Size (nanopores): 70.16 +/- 19.53 nm
- Pore Size (micropores):
- Pore morphology: Standard
- EDS: N/A
- Chip and Membrane Appearance:
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- For more information visit: https://rochester.box.com/s/1iwo0oqv38hudf101valvor94mh6hb9p