Wafer #240919-03 – 3 μm Dual Scale – Low Porosity

Manufacturer’s Data

  • Delivery Date: 2/5/2024 (picked up and logged by Ahmet Gurcan)
  • Membrane Type:  NPN 3 micron Dual Scale
  • SKU: DSSN100-1L-3.0-A1 (0.625% Porosity – Not real porosity)
  • Lot Number: 240919-03
  • Quantity Received: 230
  • Manufacturer Test Report:
    • Average Porosity (nanoporosity): 27.2%
    • Average Diameter (microporous): 2.84 μm
    • Average Diameter (nanoporous): 49.1 nm
    • Average Flux @ 1 PSI: 0.143
    • Average Flex @ 2 PSI: 0.252
    • Average Burst Pressure (PSI): 2.476
  • Packing slip & invoice: None

UR Testing

  • Average Porosity (nanoporosity): 14.22%
  • Average Porosity (microporoisty):
  • Pore Size (nanopores): 67.42 +/- 18.07 nm
  • Pore Size (micropores):
  • Pore morphology: Standard
  • EDS: N/A
  • Membrane dimensions (flat surface): 0.7 mm x 2 mm
  • For more information visit: https://rochester.box.com/s/buktwgh69du3vxyjzr6jfwh5ujgbgjrw

 