PEG microarray on oxide membrane

We have had success cross-linking PEG to TEOS membranes pretreated with TPM to aid in adhesion. This was done first on nonporous membranes, and then porous. We used 50% PEG at 1.5% cross-linker, which cross-linked at 8000ms. For comparison, 100% PEG at 3% cross-linker cross-linked at 5500ms.

Chip Schematic

Nonporous TEOS

50 pegdi 10x 8000ms_scalebar 50 pegdi 4x 8000ms_ 0z

Bottom image is at 4x. The TPM works very well to keep the PEG attached to the membrane. Will continue working on optimizing the cross-linking process, as some features do seem to be filled.

Porous TEOS  (Accidentally pulled membrane out of chip)

50 pegdi 4x 8000ms_ 50 pegdi 20x 8000ms_ scalebar

Top image is at 4x. There appear to be air bubbles, but overall the process was successful in attaching PEG to the porous membrane.