Discoloration – New wafers 2

Last week, I looked at discoloration with different wafer numbers (639,670,672,683,685,702,703), pre- and post-rebuild.  This experiment was done in the oven at 37C, in PBS and without RTP.

 

Based on the starting color, w670 and w672 are the thinnest membranes.  These discolored rather quickly (1 day).  The only other membrane that discolored over 3 days in PBS was w702.  So, wafers from the rebuilt system may not be inherently more unstable than older wafers.

Similar Posts

3 Comments

  1. Which #’s are pre and which are post? Also this is done at 37C. Jess’ discoloration was at RT. We expect the problem to be worse at 37C, right?

  2. I actually can’t keep track of which are pre and post build.  I think all of them except w639 are post-build.
    Should be worse at 37C compared to 25C.