Wafer #5240- 0.5 μm Microporous

Manufacturer’s Data

  • Delivery Date: 7/26/2024 (picked up and logged by Ahmet Gurcan)
  • Membrane Type:  MPSN 0.5 Microporous
  • SKU: MPSN400.C-3LX.1-0.5L1
  • Lot Number: 5240
  • Quantity Received: 50
  • Manufacturer Test Report:
    • Pore Size: 518.74
    • Flow Data Avg in SLPM
      • 2psi: 1.68
      • 4psi: 3.587
      • Burst: 24.28
  • Packing slip & invoice: None

UR Testing

  • Pore size: 0.48 ± 0.1
  • Pore morphology: Smooth
  • 3 Membranes from this lot were removed for QC measurements
  • Chip and Membrane Appearance – (Box-Folder: https://rochester.box.com/s/ltg1b2gbim5x0ehtfum8ds2tie2faoc4).
  • Membrane dimensions (flat surface): 0.7 mm x 2 mm
  • Representative membrane Image: See Below.

Experiences

Similar Posts