Wafer #1550 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 8/16/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100.C-1LZ.0
- Lot Number: 1550
- Quantity Received: 240
- Manufacturer Test Report:
- Pore Size: 32.9 nm
- Porosity: 19%
- Flow Data Avg in SLPM
- 2psi: 0.113
- 4psi: 0.226
- Burst: 5.45
UR Testing
- Porosity: 11.27%
- Pore size: 55.7 +/- 17.9 nm
- Pore morphology: Standard
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Chip and Membrane Appearance – (Box-Folder: https://rochester.box.com/s/y6qo37uh9khooqu82mtbqbili49xs7n1).
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- Representative membrane Image: See Below.
Experiences