Wafer #1510- 2 Slot NPN Standard
Manufacturer’s Data
- Delivery Date: 10/8/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: 2 Slot NPN – Standard
- SKU: NPSN100-2L
- Lot Number: 1510
- Quantity Received: 220
- Manufacturer Test Report:
- Avg flux SLPM at 2PSI: 0.301
- Avg flux SLPM at 4PSI: 0.606
- Avg Burst Pressure: 5.919
- Average porosity: 14.9%
Avg pore size: 52.9 nm
- Packing slip & invoice: None
UR Testing
- Porosity: 11.74%
- Pore size: 50.49 +/- 12/13 nm
- EDS: N/A
- Chip and Membrane Appearance
- Box Folder with more images https://rochester.box.com/s/65v3d1ljq0cmhe0pqvlfdgr2mbd1ae2v
- Membrane dimensions (flat surface): 2 x 0.7 mm x 2 mm
- Representative Membrane Image:
Experiences
- Cell culture
- N/A as of 10/8/2024
Manufacturer’s Missing Data:
Average porosity: 14.9%
Avg pore size: 52.9nm