Wafer #240803-10 – 2 Slot NPN

Manufacturer’s Data

  • Delivery Date: 12/18/2024 (picked up and logged by Ahmet Gurcan)
  • Membrane Type:  NPN 2 Slot
  • SKU: NPSN100-2LWMS
  • Lot Number: 240803-10
  • Quantity Received: 60
  • Manufacturer Test Report:
    • Pore Size: 54.2
    • Porosity: 16.4
    • Flow Data Avg in SLPM
      • 2psi: 0.541
      • 4psi: 0.665
      • Burst: 5.136

UR Testing

  • Porosity: 14.76%
  • Pore size: 55.13 +/- 14.79 nm
  • Pore morphology: Standard
  • EDS: N/A
  • 3 Membranes from this lot were removed for QC measurements.
  • Chip and Membrane Appearance – (Box-Folder: https://rochester.box.com/s/z8054fppdsf3hp6fybj4apx2izecr9ou).
  • Membrane dimensions (flat surface): 2 x (0.7 mm x 2 mm)