Wafer #240803-15 – 1 Slot NPN
Manufacturer’s Data
- Delivery Date: 12/23/2024 (picked up and logged by Ahmet Gurcan)
- Membrane Type: NPN 1 Slot
- SKU: NPSN100.C-1LZ.0
- Lot Number: 240803-15
- Quantity Received: 340
- Manufacturer Test Report:
- Pore Size: 57 nm
- Porosity: 17%
- Flow Data Avg in SLPM
- 2psi: 0.197
- 4psi: 0.377
- Burst: 4.618 PSI
UR Testing
- Porosity: 12.18%
- Pore size: 58.15 +/- 17.95 nm
- Pore morphology: Standard
- EDS: N/A
- 3 Membranes from this lot were removed for QC measurements.
- Membrane dimensions (flat surface): 0.7 mm x 2 mm
- For more information visit: https://rochester.box.com/s/9pn2a46e574p4kzxbmynr53y0dz3m5f0