ZO-1 staining of confluent RPE cells on various MgF2 substrates

I’ve been culturing RPE cells over here in Rochester for my MgF2 fabrication paper, in which the goal is to make a permeable Raman compatible cell substrate. My previous work had shown polarization of RPE cells (via-ZO-1 staining) on nanoporous MgF2 nanomembranes, but in the meantime, I have reworked my MgF2 substrates to be thicker and stronger, with larger 400 nm pores. I cultured P6-P8 cells on a variety of substrates (high porosity chips (1:1 spacing), glass coverslips coated with MgF2, silicone, TCP) for 22 days. These were then fixed and stained for ZO-1. None of these membranes broke during culture.

 

Previous Results

nanoporous MgF2 (no coating) shows polarization on the active area, and not really surrounding it. Staining wasn’t great. The permeable transwell shows ZO-1 Polarization.

 

nanoporous MgF2 Substrate coated with PLL shows significant ZO-1 staining. Tissue culture plastic doesn’t show significant polarization. The polarization also extends well beyond the boundaries of the permeable region.

 

Treatments

  • TCP
    • null
  • Microporous MgF2 (2o0 nm thick, High Porosity, 1:1 400 nm pores, 100 micron square windows)
    • + .01% PLL
    • null
  • Coverglass coated with MgF2 (200 nm thick, not permeable)
    • + .01% PLL
    • null
  • Silicone (cells that spill over onto the silicone gaskets)
    • null

 

Devices

Devices used in this experiment. Chips were fabricated to fit in a 6 well plate, using ozone bonding to adhere the chips to the bottom gasket. The top gasket was only affixed with stiction.

 

Procedures

  • 1/9/17
    • Devices were autoclaved
    • Seeded P6 RPE cells at 5000 cells/mm^2 in flat devices
      • wanted about 50 cells in 100 um square window, resulted in 35,325 cells/well,
      • Observed about 30-40 cells in a window immediately after seeding
    • Cells were fed 3x a week
      • RPE Complete Media = DMEM + sodium pyruvate + L-glutamine + 10% FBS
    • Imaged 1x a week (phase)
  • 1/18/17
    • Cells on the MgF2 coverslip all died. Reseeded P8 RPE cells on the coverslip after washing with 1x PBS.
  • 2/1/17 – Fixation and staining
    • Aliquot Antibodies
      • F0382 SIGMA Secondary antibody: Anti-Rabbit IgG (whole molecule)–FITC antibody produced in goat affinity isolated antibody, buffered aqueous solution
        • use at 1:80-1:50 dilution
        • Aliquot 2ML into 50x 40UL portions
        • to Make 2000uL of stain (1:50), add aliquot to 1960ul of solution (1%BSA in PBS)
      • HPA001636 SIGMA Primary Antibody: Anti-TJP1 antibody produced in rabbit Ab1, Prestige Antibodies®Powered by Atlas Antibodies, affinity isolated antibody, buffered aqueous glycerol solution
        • Use in 1:200 dilution for immunohistochemistry
        • Aliquot 100uL into 10x 10uL portions
          1. To make 2000uL of stain, add aliquot to 1990 uL of solution (1%BSA in PBS)
          2. This is enough stain for 2000uL/150uL = 13 devices
    • Prepare Solutions
        1. 1% Triton X-100 in PBS
        2. 4% PFA in RPE Media
        3. 2mL of Primary antibody
        4. 2mL of secondary antibody (following day)
    • Fix Cells (22 days)
      1. Wash devices with 1x PBS
      2. Fix with 4% PFA in warmed Cell media (37C) for 30 minutes in fume hood
      3. Wash Devices with 1x PBS 3 times
    • Permeabilize + Stain Cells
      1. Permeabilize with Triton X-100 (0.1% in PBS) for 15 minutes at room temperature
      2. Wash with 1x PBS
      3. 1% BSA in PBS for 1 hr to block aspecific binding
      4. Wash with 1x PBS 2 times
      5. Add Rabbit-Antihuman ZO-1 antibody (150uL of 1:200 diluted antibody, 10 ug/uL) to device, and incubate overnight in the fridge
      6. The following day, wash with 1x PBS 3 times
      7. Add secondary antibody FITC-antigoat (150 uL of 1:50 diluted antibody) for 1.5hrs
      8. Wash with 1xPBS 3 times and submerge devices in PBS
      9. Store in Fridge

Mounting and Imaging

I removed the silicone gaskets surrounding each of wells and flipped over the devices to image in a small dish (immersed in 1x PBS).

Results

Surprisingly, the MgF2 coated material all seem to have ZO-1 expression, including the non-porous coverglass. The silicone and TCP do not.

 

20x Microporous Chip null-coated. The ZO-1 stains aren’t quite in the same plane.

 

10x Microporous chip +PLL coating. ZO-1 extends everywhere in the well.

20x D21 P8 RPE cells on null-coated MgF2 coverglass, showing ZO-1 expression. The PLL well sloughed off the coverglass when mounting (like a tissue biopsy).

 

Future

I believe my washing steps could be better. The amount of fluorescence is pretty low in all of these images. I am also going to use larger gaskets that can access more media at once.

 

Devices assembled by Tom Andolsek. Both high porosity and low porosity variants are available.