Wafer #1520 – 3 micron Dual Scale – Low Porosity

Manufacturer’s Data

  • Delivery Date: 12/8/2023 (picked up and logged by Ahmet Gurcan)
  • Membrane Type:  NPN 3 micron Dual Scale
  • SKU: DSSN100-1L-3.0-A1 (0.625% Porosity – Not real porosity)
  • Lot Number: 1520
  • Quantity Received: 220* (SimPore said it should be 240 – confirming details as of 12/8/2023. SimPore said it should be 220 on 12/11/2023)
  • Manufacturer Test Report: Average (NPSN) Porosity:17.7%, Average Diameter: 60nm
  • Packing slip & invoice: None

UR Testing

  • Porosity: 20.9 +/- 1.2%
  • Pore size: 74.7 +/- 2.2 nm
  • Pore morphology: Standard
  • EDS: N/A
  • Chip and Membrane Appearance:
  • Membrane dimensions (flat surface): 0.7 mm x 2 mm
  • Full Test Report / Images in Box: See Below for Image:
  • Representative Box Image: See Below

Experiences

  • Cell culture
    • Michelle: Not used as of 12/8/2023

Similar Posts